You forgot about the “cold pull” method! That’s the easiest and best. There is a version below talking about doing a nylon-cold-pull but any filament will do.

Heat the filament a bit below printing temp (200C is fine for ABS or PLA) and shove some filament in there so there is good contact (this is in case there was a retraction). Then cool the head to the “cold pull” temperature (about 90C for PLA and 120C for ABS but temperatures can vary by 60C depending on nozzle design and filament diameter). Then pull real hard on the filament. It should take at least 1kg force - usually more like 5kg or 10 pounds. If it comes out too easily then lower the temp. If it doesn’t come out at all raise the temp until you learn proper cold pull temp for your nozzle and plastic.

It should come out in the exact shape as the inside of the nozzle. Complete with black specs of gunk and any cloggint things like sawdust or dust.