Go to homepage
3 / 8
Aug 2015

Hi guys,

I’ve been trying to print with PP filament and I’m experiencing major problems with getting it to stick to the print bed. I have printed both with new PP filament and filament that I produced myself using a Filabot extruder from new PP pellets.

As you can see in this picture it is not only sticking that’s the problem but a combination with a lot of warping as well.

I’ve tried the following things:

- Heated bed temperature of 0, 60, 80, 100 degrees C

- Special PP printplate

- BuildTak plate

- Applying glue stick to print bed

- Extrusion temperatures of 245C and 225C

Does anyone have experience with printing PP or a good solution? Thanks a lot!

Cheers,

Bram

  • created

    Aug '15
  • last reply

    Nov '15
  • 7

    replies

  • 4.4k

    views

  • 5

    users

Hi @bramhallo

Have you tried slowing down the print speed of the base layers? You might also feed the extruder a bit more (like 150 - 180% on the first layers. I haven’t tried PP yet, but I think it’s similar to PET.

I also had lot sticking problems with PET

3 months later

You might have solved it by now, but I recommend packing tape made of polypropylene 1000 bed and 220 extruder.