Hi all,

Getting ready to try some nylon. Looking for any advice including brand and where you got it. I am in the US so that will factor in on a vendor I guess.

Printer will be a Flashforge Creator Pro with Micro-Swiss all metal hot ends.

Taulman 230 is the easiest to go nylon wise. It is a blend, that prints similar to PLA, so that is nice.

There are really two issues that you will deal with re:nylon.

Getting it to stick to build platform–> Glass with lots of Aquanet Super Hold.

Stringing- re retraction settings.

But both are doable.

Thanks Perry, I’ll look at that. I am using a PEI bed at the moment so will see how that goes but have the trust Aquanet standing by!

It’s time to broaden my horizons on materials a bit!!

That definetly looks like a starting error. It could be a couple of things.

I think it is not purging your hot end enough before the print, so small amount of plastic gets on there, that gets pulled on the next layer. I am leaning this way, because of the direction of the pull.

I can also see you are either too close to your bed, or overextruding your first layer. This can also leave a blob when the outline meets itself when it completes the outline, again creating a situation where there is a little too much plastic, that gets picked up by the extruder on the next layer.

Definitely add or increase skirt, or raise bed a little, or print less % of first layer. This should make it go away.

This is all guessing based on the picture…

I bought some Taulman filament from Amazon. It popped and sizzled when it was printing. It had water in the filament. I took the roll to work and put it in the welding rod oven for 3 days. The welding oven maintains a temp of around 95 C. The filament prints much cleaner and better. No popping and no sizzling. The color did fade and the spool warped but the filament was OK.

I read something on nylon that it can absorb its weight in moisture in 24 hours. It also said you really need to dry it before use.

I really appreciate the advice. I need to go back to the cube and work with it. Other prints are printing nice however so hopefully it is just some adjustments/fine tuning but overall a good start with the MS hotends so I am happy so far! Hasn’t been a disaster!

If it popped and sizzled right out of the bag, first use, then something is seriously wrong. I have done a lot of it, and never had that happen.

You also said the color faded. I did not know Taulman had colors. Are you sure it was taulman.

Either way, once you open it, use it, but it back in a plastic bag with 4 dissecants, should be good.

Yeah, it popped and sizzled right out of the bag. I read reviews on Amazon with the same issue, but decided to take a chance. My buddy ordered a roll a few weeks later with the same issue. And yup its taulman. The original clear color faded to yellow.