I was experimenting with some new filament I got from winbo tech, so I changed a few of my settings around to try and fix my stringing issue. I have now set my retraction to 8 mm, my extrusion temp to 228C, and my bed temperature to 100. Does that sound like a better direction to go in?

Thanks.

I replaced the section a few days ago and I was still getting the same results… Have you ever used filament from Winbo-Tech before? That is the filament that started this issue.

Hairspray will make the difference. Kaptin tape, doesn’t work for me.

Dear Dalvin,

Forget everything you learnt from printing PLA. ABS is a hard material to print. It is very hard to print ABS with a printer without a totally closed print chamber.

What you can do:

1. Set the bed temperature to 100 - 110 C

2. Extrude at a higher temperature. We mostly extrude at 235 C but this depends on the filament you use. Lower temperatures decreases layer adhesion as it is in your case.

3. If there is any, shutdown any air condition in the room. Close the windows.

4. Do not use any nozzle fan. Shut it off. It is for printing PLA.

5. Apply a fresh layer of Elmer’s glue stick or UHU glue stick (also TESA glue stick works) to your print bed.

6. Do not expect a succesful print of a big object with ABS withou a closed chamber.